Mix epoxy base and pitch curing agent parts by volume, or weight. DO NOT THIN.
(2)
Only mix sufficient for requirements. Pot life of mix is approximately 3 to 4 hours at 68oF (20oC).
(3)
Remove damaged coating(s) until the aluminum surface is reached.
(4)
Roughen surface with crocus cloth.
(5)
Apply coat of epoxy pitch at approximate rate of 4 1/2 oz/yd2 (150 gm/m2), and allow to air dry for
approximately thirty minutes.
(6)
Liberally cover epoxy pitch coating with bauxite grit at an approximate rate of 3 Ib/yd2 (1500 gm/m2), and
allow coating/bauxite grit to dry for twelve hours.
(7)
Lightly brush off any loose grit.
(8)
Apply further coat of epoxy pitch at approximate rate of 20 oz/yd2 (750 gm/m2), and allow seven days to
cure.
(9)
Stacking is permitted during the seven day period, provided that no contact is made with the treated
surface.
8-41 (8-42 blank)